英国标准室温和高温用承压铸钢的高温屈服强度
发布时间:2007-12-16 14:45:54点击率:
技术类别:机械技巧
|
钢 号 |
数字 牌号 |
热处理 代号① |
铸件厚度 ≤/mm |
下列温度的高温屈服强度σ0.2/MPa | |||||
| 100℃ | 200℃ | 300℃ | 400℃ | 500℃ | 550℃ | ||||
| GP240GR | 1.0621 | +N | 100 | — | — | — | — | — | — |
| GP240GH | 1.0619 | +N | 100 | 210 | 175 | 145 | 130 | — | — |
| +QT | 100 | 210 | 175 | 145 | 130 | — | — | ||
| GP280GH | 1.0625 | +N | 100 | 250 | 220 | 190 | 160 | — | — |
| +QT | 100 | 250 | 220 | 190 | 160 | — | — | ||
| G20Mo5 | 1.5419 | +QT | 100 |
— |
190 | 165 | 150 | 135 | — |
| G17CrMo5-5 | 1.7357 | +QT | 100 |
— |
355 | 230 | 200 | 175 | 160 |
| G17CrMo9-10 | 1.7379 | +QT | 150 | — | 244 | 345 | 315 | 280 | 240 |
| G12CrMoV5-2 | 1.7720 | +QT | 100 | 264 | 385 | 230 | 214 | 194 | 144 |
| G17CrMoV5-10 | 1.7706 | +QT | 150 |
— |
385 | 365 | 335 | 300 | 260 |
| GX15CrMo5 | 1.7365 | +QT | 150 |
— |
390 | 380 | 370 | 305 | 250 |
| GX8CrNi12 | 1.4107 | +QT1 | 300 | — | 275 | 265 | 255 | — | — |
| +QT2 | 300 | — | 410 | 390 | 370 | — | — | ||
| GX4CrN13-4 | 1.4317 | +QT | 300 | 515 | 485 | 455 | — | 340 | 290 |
| GX23CrMoV12-1 | 1.4931 | +QT | 150 | — | 450 | 430 | 390 | — | — |
| GX4CrNiMo16-5-1 | 1.4405 | +QT | 300 | 515 | 485 | 455 | — | — | — |
① 热处理代号:N—正火;Q—淬火,T—回火。热处理温度同表5-140。
(2)英国BS标准低温用承压铸钢[BS EN 10213-3-1995]
a.低温用承压铸钢的钢号与化学成分,见表5-142